I:Principium Core munus implementation
Anti UV Polyester Dope dyed Filamentum yarn Achieves a tutela effectum (upf valorem ≥ 50) by introducendis UV absorbers (ut benzophenones et Benzotriazoles) in fibris, convertens UV radiationi, in industria aut humilis-uvam radiationi. Combination de tyeing et anti UV munus necessitates ad statera stabilitatem et compatibility utriusque.
II,Detailed Explicationem Key Productio processibus
(I)Rudis Material Pretreatment et Modification
Electio UV absorbers
Iudicium: Particulae magnitudine ≤ I μ M (ut vitare spheara blockage), scelerisque stabilitatem ≥ CCLXXX ℃ (altum temperatus resistentia pro polymeriza), bonum compatibility cum polyester (ut ne praecipitatio).
Genus:
Organicum parva moleculae absorbents (ut UV-DXXXI): Introduced per mixtum tincto, cum effusio unam 290-400nm.
Nano Pulveres (ut tio ₂, ZNO): Cum particula magnitudine 50-100nm, augendae praesidium per sparsas ultraviolet lux, et requirere superficiem immutatio (Silanene copulatis agente curatio) ad amplio dispertibility.
Praeparatio polyester crustae
Modificatio Modification: Per Polyester Melt Polymerization scaena (vel post solidum-statu polymerization), UV absorbent masterbatch additur ad rationem 0,5% -2% et uniformiter dispersit per geminae -2% et uniformiter dispersit per geminae -2 et uniformiter dispersit per Didymus -2 et uniformiter dispersit per geminae -2% et uniformiter dispersit per geminae -2 et uniformiter dispersit per Didymus -2 et uniformiter dispersit per geminae -2 et uniformiter dispersit per Didymus -2 et uniformiter dispersit per Didymi -2 et uniformiter per Didymus -2 et extruditor in uniformiter in Dispersit.
CO Polymerization Modification: Monomers quibus UV absorbing coetibus (ut Benzotriacoly P-Hydroxybenzoate) sunt incorporatus in polyester Molecular vincula ad consequi permanens UV resistentia (excelsum sumptus, idoneam ad summus finem products).
(II)Spheara et extendens processus
PARAMERIUM
Temperamentum: Meltentur spheip temperatus est 285-300 ℃ (5-10 ℃ altior quam Ordinarius polyester) ad vitare corrumpuntur vel agglomerationem de absorbent.
Celeritate: High Volo spheara (4000-5000 m / min) combined cum denario (15-50 dtex) ad augendam fibra specifica superficies et augendae UV effectus.
Extendens et effingens Optimization
Extendens Ratio: 3.5-4.0 temporibus, amplio fibra crystalliness (Crystallination ≥ XLV%), reduces amorphous defectus, et vitat UV penetratio.
Calor occasum temperatus: 180-200 ℃ (10-20 ℃ inferior quam Ordinarius Polyester), ut ne scelerisque decomposition of absorbent et imperium DECREMENTUM Rate ≤ VIII%.
(III)Dyeing processus (clavis compatibility imperium)
Electio de Tydeing modi
Rudis liquorem coloring + UV repugnant miscent: Antequam spheara, pigmento masterbatch et UV absorber sunt additae eodem, idoneam ad tenebrosum products (Nigrum, classis hyacintho, etc., et pigmento se potest adiuvaret in umbra), cum color Fastess ≥ IV campester et longa, cum Colo colore.
Post macia + anti UV consummatione:
Disperse Dyes debet esse in altum-temperatus et summus pressura tyde (CXXX ℃ × 30min), et moritur cum bono compatibility cum absorbents debet esse electus photochemical et absorbents inter anthrhquanone, ad vitare photochemical et absorbents).
Post Tydeing, intinge volvens anti ultraviolet consummatione agente (ut aqua-fundatur UV absorbent Suspendisse) est apta lucem color products, sed ejus baptismata a XX post V temporibus baptismata).
Optimization de Dyeing Processus
Ph potestate: PH de tinctura balneum est 4.5-5.5 (debiles acidic) ne absorbent a decomposing sub alkaline conditionibus (ut Benzophenones facile hydrolyzed ad PH> VII).
ELOGIUM electio: Addere non-Ionic adtritio agentibus (ut pingue alcohol Polyoxyethylene aether) ad vitare causam repulsu inter Ionic additives et absorbents, quae potest affligit.
(IV)Eget Synergy Imperium
Et commercium inter absorbent et tinctura
UV absorbers ut certet cum Dyes ad binding sites in fibris, ducens ad decrementum in tyeing profundum (k / s valorem reducitur X% -15%), quod opus est compensatur per augendae tinctura dosis aut optimizing in formula.
Exempli gratia, cum tydeing altum hyacintho, moles Ordinarius Polyester Dye usus est II% (owwf), et moles UV repugnant polyester necessitates ad augeri ad 2.5% -3% (mwf).
Melius lux ieiunium
UV absorbers potest adiuvaret in meliorem lucem ieiunitas Dyes (ut augendae lucem resistentiam campester of Rubrum LX tinctura in UV repugnant fibris ex gradu III ad gradu ad mori moleculis in Damno Damnofer IV.
III,Technologia difficultates et solutions
Pauper disperii absorbent
Problemaaa: Agglomeration ducit ad spheering fractio
Solution: Nano Technology adopting Nano molere (molendini cum harenae D50 ≤ 500nm) + superficiem immutatio (ut coating tio ₂ cum stearica acidum).
Insufficiens uniformitatem adipiscing
Problemaaa: Butbents afficiunt ad tyeing rate dyes, ducens ad discoloration.
Ratio: Segmeted calefactio et tydeing (ut calefactio ad I ℃ / min pro 30-60 ℃ et II ℃ / min pro 60-130 ℃), extendens ad XL minutes.
Eget diuturnitatem
Problemaaa: Pauper baptismata resistentia anti UV agentibus post consummatione.
Solution: Reactive absorbents (ut UV absorbents continet epoxy coetus) sunt ad covalently vinculum cum fibris per crucem-vinculum reactiones, cum washabiling in ≥ XX temporibus.
IV:Applicationem missionibus et processus adaptatione
Velit vestimentum: Prior sit datum ad processus of fuco cum originali solutione et miscent absorbents, accipit in rationem UV praesidium et color fastidess (ut hiking vestimenta et solutario vestimenta).
Indoor ornamentum: Post consummatione anti UV + Dyeing processus, cum inferiori (ut tanquam aulaea, sunshades), sed requirit iusto sustentationem.
Medical commeatus: Co mutatio et originale liquorem fuco ad vitare absorbent migrationem (ut chirurgicam togis et fontes), in obsequio cum medical gradu salus signa.